THYOSIL E1560


Waterborne Acrylic Resin 水性丙烯酸树脂


Description 描述

THYOSIL E1560 can be formulated into primers and gloss topcoatswhich are designed for commercial, institutional, and industrial maintenancemarkets.
The high gloss capability, corrosion resistance, hardness, and chemicalresistance characteristics imparted by THYOSILE1560 in a waterborne finish are typical of those associatedwith conventional solvent-based maintenance systems.
THYOSIL E1560 可以配制成光泽面漆和底漆,用于工业和商业的防腐防锈漆 。具有高光泽,耐腐蚀,耐化学腐蚀以及高硬度等性能。是终结传统溶剂型防护漆的水性品。


Characteristics and advantages of use特性与优势

·        Excellentadhesion on metallic substrates.
·        在金属表面具有超强的附着力
·        Recommendedto apply on metal surfaces without prior treatment.
·        推荐适用于未经处理的金属表面
·        Primer formulations exhibit stability with commonlyused corrosion-inhibiting pigments.
·        底漆可以与常用防腐蚀颜料的配方呈现出良好的稳定稳定性
·        Verygood resistance to water and alcohol.
·        具有优良的防水和酒精性能


Coalescent and Co-solvent Effects 成膜助剂(聚结剂成膜溶剂的作用
Thetype and level of coalescent in the formulation is critical to the balance of properties.Hydrophobic coalescents that partition to the polymer phase are recommended asopposed to water-soluble coalescents.
成膜助剂(聚结剂)的类型和添加量的在配方中对性能的好坏是至关重要的。
常用疏水助剂为:Dowanol DPnB  二丙二醇丁醚Texanol
常用亲水助剂为: 二丙二醇甲醚 和丁基乙二醇
一般情况下天热的地区添加量要少于天冷的地区。

Flash Rust Inhibitors 闪锈抑制剂

Inwaterborne paints for steel, the water phase must be inhibited or flash rustingwill occur. The recommended additive is sodium nitrite, which is very effectiveat very low use levels.
水性涂料用于钢铁时,触水时必须抑制或将发生的闪锈。推荐的添加剂是亚硝酸钠,在非常低的使用量,是非常有效的。


Defoamers 消泡剂

Foamcontrol is a major concern in waterborne paint formulation design. Additivesare necessary to eliminate foam during manufacture and on application. Thechoice of defoamer type and level will depend primarily on the formulation andmode of application.
泡沫控制是水性涂料配方设计中的主要问题。添加剂在制造过程中,应用是必要的,以消除泡沫。消泡剂类型和级别的选择将主要取决于配方和应用模式



TypicalProperties 典型性质
Theseproperties are typical, do not constitute specifications

Appearance

White bluish emulsion 白偏蓝乳液

Solids (%)  固含量

41

pH

7,5

Viscosity a 25oC (cP)粘度

< 500

MFFT (oC)成膜温度

30

Tg (oC)玻璃化温度

40



High gloss white topcoat typicalformulation高光面漆的典型配方

Step 1) White grinding第一步: 白色色浆的研磨制备


Ingredient 成分

Percentage (%)
1

Water  
18,05
2

Dowanol DPM 二丙二醇甲醚
1,06
3

Butyl Glycol  丁基乙二醇
6,54
4

THYON PH730*
2,89
5

NH4OH (28%)
0,44
6

Wetting agent  润湿剂
0,62
7

Antifoam  消泡剂
0,62
8

Pigment - TiO2 -    钛白粉
67,63
9

Water  
2,15


Total
100,00

*Ammonia solution of resin THYON PH725.  

Step 2) High glosswhite topcoat 第二步高光白色面漆


Ingredient

Percentage (%)
1

THYOSIL E1560
64,85
2

White grinding 白色浆
23,25
3

Dowanol DPM  二丙二醇甲醚
1,51
4

Butyl Glycol 丁基乙二醇
9,30
5

Antifoam    消泡剂
0,05
6

Flash rustinhibitor 闪锈抑制剂
0.89
7

NH4OH (28%)
0,05
8

Wetting agent    润湿剂
0,10


Total
100,00


Safe handling Information
Before using thisproduct, read carefully the Material Safety Data Sheet (MSDS).


Note: The statements above are based on the current state of knowledge. They are intended to describe the product inrelation to necessary safetyprecautions, and should not be used as awarranty of any specific property. Revision: May2013.